Ref. | Cement (kg/m3) | GSA (kg/m3) | FA (kg/m3) | CA (kg/m3) | Water (kg/m3) | Curing period (days) | Strength (MPa) | No. of data |
---|---|---|---|---|---|---|---|---|
Abro, Kumar et al. [2] | 264–310 | 0–46.5 | 620 | 1240 | 155 | 3, 28 | 13.2–36.9 | 12 |
Alabadan, Olutoye et al. [4] | 155–310 | 0–155 | 620 | 1240 | 171 | 7, 14, 21, 28 | 2.3–31.4 | 24 |
Buari, Olutoge et al. [8] | 276–460 | 0–184 | 650 | 1068 | 170 | 7, 14, 28 | 9.8–49.0 | 15 |
Dharani and Selvan [12] | 263–376 | 0–113 | 636 | 1103 | 177 | 7, 28 | 11.1–29.0 | 12 |
Kanchidurai, Nanthini et al. [28] | 314–392 | 0–78.4 | 477 | 1353 | 216 | 7, 28 | 19.9–29.8 | 10 |
Karthikeyan, Saravanan et al. [29] | 309–425 | 0–106 | 510 | 1234 | 234 | 7, 14 | 5.5-29.1 | 12 |
Krishnan and Nizar [31] | 326–383 | 0–57.5 | 549 | 1184 | 192 | 7, 14, 28 | 7.2–30.1 | 21 |
Ige, Anifowose et al. [18] | 248–310 | 0–62 | 620 | 1240 | 186 | 7, 14, 28 | 10.5–24.3 | 15 |
Ikumapayi, Arum et al. [19] | 260–310 | 0–49.6 | 620 | 1240 | 186 | 7, 28 | 12.6–16.3 | 14 |
Lakshmi and Sagar [32] | 202–310 | 0–109 | 620 | 1240 | 186 | 7, 14, 28 | 5.9–23.2 | 24 |
Mujedu and Adebara [35] | 77.5–310 | 0–233 | 620 | 1240 | 171 | 7, 28 | 1.8–26.7 | 24 |
Nwofor and Sule [36] | 186–310 | 0–124 | 620 | 1240 | 171 | 7, 14, 21, 28 | 2.0–25.5 | 20 |
Ogork, Uche et al. [37] | 191–318 | 0–127 | 705 | 1252 | 175 | 7, 28, 60, 90 | 5.5–31.1 | 24 |
Pandi, Ganesan et al. [39] | 289–385 | 0–96.3 | 577 | 1154 | 193 | 28, 56, 90 | 18.2–26.0 | 18 |
Raheem, Oladiran et al. [44] | 264–368 | 0–73.6 | 620–846 | 956–1240 | 171–202 | 7, 14, 21, 28 | 8.2–35.1 | 28 |
Samuel [46] | 353–470 | 0–118 | 705 | 940 | 282 | 3, 7, 21, 28 | 4.8–26.3 | 24 |
Overall | 77.5–470 | 0–233 | 477–846 | 940–1353 | 155–282 | 3–90 | 1.79–49.0 | 297 |