Skip to main content

Table 7 Test results of concrete strength (Mpa)

From: Influence of steel plates on the compressive strength and pore structure of concrete

 

3 days

7 days

28 days

C20-R0

14.6

18.5

23.5

C20-R1

14.0

17.7

21.5

C20-R2

13.2

15.5

19.5

C20-R3

12.3

14.5

18.6

C20-R4

12.2

13.5

16.0

C20-R5

8.9

12.5

16.1

C20-R6

8.6

11.9

15.4

C20-R7

8.9

11.6

14.6

C20-R8

7.0

10.1

12.5

C50-R0

38.4

45.0

52.0

C50-R1

35.6

43.5

51.5

C50-R2

29.6

42.7

47.6

C50-R3

27.8

40.8

44.3

C50-R4

25.4

38.5

42.4

C50-R5

23.5

36.5

41.5

C50-R6

21.1

30.1

37.6

C50-R7

19.8

28.9

32.5

C50-R8

17.5

26.5

30.5