Table 6 Welding procedure conditions

From: Effect of welding parameters on the mechanical and metallurgical properties of armor steel weldment

Base metals

Armox 500T

Thickness of plate

10 mm

Welding process type

GTAW

Welding machine type

Fronius Magic Wave 3000

Filler metal type

AWS A5.18 ER 70S-6

AWS A 5.9 ER 307

AWS A 5.18 ER 70S-6

AWS A 5.9 ER 307

Joint type and angle

Single V (60°) and single bevel (30°)

Filler wire diameter (mm)

2.4

1.6

2.4

1.6

Gas (%)

100% argon

Gas flow rate l/min

10 l/min

10 l/min, back shield 8 l/min

10 l/min

10 l/min, back shield 8 l/min

Welding method

Continuous

Not continuous

Cooling method

Without cooling (left at ambient temperature after completion of the whole welding)

With using compressed air (6 bars) in the cooling after each pass up to 100 °C